Technical Data Sheet #36
We’ve all seen it at some point: galvanized steel whose appearance can vary greatly from that of the adjacent piece. The thickness of the zinc coating can also vary considerably between two galvanized parts.
To understand why both the zinc coating thickness and the appearance of the zinc coating can vary so much between two different profiles, we’ll examine what happens when an object is immersed in the zinc bath. In doing so, we’ll delve deeper into the influence of steel composition, bath temperature, and the formation of the various zinc-iron alloy layers. In this fact sheet, we explain the relationship between the characteristics of the zinc coating and the composition of the steel.
As early as 1742, hot-dip galvanizing was described as the most effective method for protecting steel against corrosion. The zinc coating completely envelops the steel, and thanks to zinc’s very low corrosion rate, this method can easily provide maintenance-free protection for 50 to 100 years
(See also Technical Information Sheet 10: Corrosion Resistance of Hot-Dip Galvanized Steel).
What is often less well known is that hot-dip galvanizing involves much more than simply applying a layer of zinc to steel. During immersion, a metallurgical process takes place in which zinc and iron diffuse into one another. This creates various iron-zinc alloy layers, which are typically covered by an outer layer of pure zinc (the solidification layer).
A key advantage of this process is that the reaction is not affected by the object’s geometry, such as sharp edges. As a result, a zinc coating of similar thickness forms on sharp edges as on the rest of the object.
DIFFUSION EXPLAINED
Hot-dip galvanizing is a process in which atoms move from an area of high concentration to an area of low concentration, a phenomenon known as diffusion. During this process, zinc atoms penetrate the steel, while iron atoms move toward the molten zinc. This results in a phase transformation, during which new compounds are formed between iron and zinc: the so-called zinc-iron alloy layers. Each alloy layer has a unique crystal structure, which gives it distinct properties and ensures a strong bond between the steel and the zinc. The result? A durable protective layer that significantly extends the steel’s service life.
In this document, we describe the formation of the zinc coating at a galvanizing temperature of approximately 450°C (440–460°C). Galvanizing at higher temperatures is also possible, but is not discussed here. This method is known as *delta galvanizing*, a term that—not coincidentally—refers to the zinc coating formation discussed later in this document.
In order to galvanize an object, the zinc must be in a liquid state. This occurs above its melting point of 419.5°C. Iron, on the other hand, does not become liquid until 1,538°C. It is precisely this large difference in melting temperatures that allows intermetallic alloy layers of iron and zinc to form during the galvanizing process.
As shown in the phase diagram above, the iron-zinc alloy can exist in different phases at a zinc bath temperature of approximately 450 °C. We will not delve deeper into all the underlying mechanisms, as this topic could easily fill an entire book. Therefore, below is a brief summary of the most important steps in zinc coating formation:
When the object is immersed in the zinc bath, two zinc-iron alloy layers are formed: the delta layer and the zeta layer. At a temperature of approximately 450 °C, the solubility of zinc in iron increases significantly, causing the steel surface to become saturated with zinc. The gamma layer then forms at this interface. In reality, this consists of two very thin layers. In a micrograph of the zinc coating, these gamma layers are usually barely visible. The alpha phase is located directly at the steel surface.
When the object is lifted out of the zinc bath, the zinc layer is covered by an outer layer of pure zinc: the eta layer. This layer is also known as the solidification layer. Depending on the composition of the steel, this pure zinc layer can sometimes react further within a short time and be converted into a zinc-iron alloy layer.
Under certain conditions, the galvanized coating may cool only slowly after being lifted out of the zinc bath, for example in structures with hollow sections. This can cause saturation in the gamma layer. As a result, a gap will form between the steel surface and the gamma layer, causing the galvanized coating to detach locally from the substrate.
This phenomenon is attributed to the so-called Kirkendall effect. Put simply, saturation occurs at the surface of the ferritic iron structure due to the diffusion of iron atoms. This creates “gaps” between the gamma layer and the steel surface.
CHEMICAL COMPOSITION OF THE STEEL
The silicon content of the steel and, in certain cases, the phosphorus content as well, determine the reactivity of the diffusion reaction during hot-dip galvanizing. Steel with a relatively high silicon content generally exhibits higher reactivity, resulting in a thicker zinc coating than steel with a lower silicon content.
For steel grades with a particularly low silicon content, phosphorus also plays an important role in the formation of the zinc coating and its properties (see Technical Information Sheet 18: Influence of Chemical Composition on Zinc Coating Formation).
EFFECT OF IMMERSION TIME ON ZINC COATING THICKNESS
The formation of the zinc coating is largely determined by the composition of the steel. It is important to note that steel with a relatively high silicon content is particularly reactive. With these types of steel, the diffusion reaction continues throughout the immersion, causing the zinc coating thickness to increase as the immersion time lengthens. Heavy, thick-walled steel objects take longer to reach the temperature of the zinc bath. As a result, they remain in the zinc bath longer and, given the same chemical composition, typically develop a thicker zinc coating than thinner steel parts. The difference in zinc coating thickness can amount to several tens of micrometers.
Remarkably, this does not apply to steel with a particularly low silicon content. For such steel grades, the immersion time has only a limited effect on the final zinc coating thickness. In practice, the difference is often no more than about 10 micrometers.
As soon as an object leaves the zinc bath, the diffusion process does not stop immediately. Although this may sound surprising, the reaction between zinc and iron continues for some time during the cooling phase. The diffusion process, which begins at approximately 450 °C and is responsible for the formation of the zinc-iron alloy layers, continues even after the object has been removed from the zinc bath. Only when the temperature drops to approximately 200 °C does the diffusion slow down to the point where practically no further structural changes occur. A characteristic of low-silicon steel is that the typical zinc-iron alloy layers evolve only to a limited extent during this cooling phase. This is because such steel grades are not very reactive, both during galvanizing and during the subsequent cooling.
In steel with a high silicon content—also known as reactive steel—significant structural changes do occur during cooling. Because the material is no longer in contact with the molten zinc bath during this phase, no new zinc atoms can be supplied. However, the reaction continues, with zinc atoms from the pure zinc layer (the eta layer) being consumed for the further formation of zinc-iron alloy layers.
As a result, part of the original pure zinc layer is converted into a zinc-iron alloy layer. Consequently, an initially shiny, silver-colored zinc layer may change into a duller, grayish zinc layer during cooling.
EN ISO 14713 part 1
Zinc coatings – Guidelines and recommendations for the protection of iron and steel in structures against corrosion – Part 1: General design principles and corrosion resistance.
EN ISO 14713 part 2
Zinc coatings – Guidelines and recommendations for the protection of iron and steel in structures against corrosion – Part 2: Hot dip galvanizing
TECHNICAL DATA SHEET 10
Corrosion Resistance of Hot-Dip Galvanized Steel
TECHNICAL DATA SHEET 12
The Mechanical Properties of Hot-Dip Galvanized Steel
TECHNICAL INFOBLAD 18
Influence of chemical composition on zinc coating formation
TECHNICAL DATA SHEET 21
Hot-dip galvanizing of MC steel
TECHNICAL DATA SHEET 22
Hot-dip galvanizing of cut edges
TECHNICAL DATA SHEET 25
Zinc Patina: Formation and Protection
TECHNICAL DATA SHEET 26
Ensuring the Adhesion of the Zinc Coating